Quick answer: Install GRP grating by clipping to steel supports with SS304/316 G-clips (never weld), torque M8 to 8-12 N-m and M10 to 15-22 N-m, leave 3-5 mm expansion gaps, and seal every cut edge with resin gel-coat within 30 minutes.

Tools and preparation

GRP grating is installed by bolting or clipping to a steel substructure — never by welding. You will need: SS304 or SS316 G-clips or S-clips, M8/M10 stainless bolts, a torque wrench (8–22 N·m), a diamond-tipped saw or carbide cutting disc, measuring tape, and safety gear (gloves, goggles, dust mask). Cut edges must be sealed with resin gel-coat to prevent water ingress into the glass fiber.

Step-by-step installation

  • 1. Verify substructure. Support beams must be level, clean and within specified spacing (typically ≤ 1.2 m for 38 mm molded, ≤ 2.0 m for 50 mm pultruded I-bar).
  • 2. Pre-drill and fit clips. Place a clip at every support intersection — minimum 4 clips per panel. Do not over-tighten; torque M8 to 8–12 N·m, M10 to 15–22 N·m.
  • 3. Leave expansion gaps. Allow 3–5 mm gap between panels; on runs longer than 3 m or operating above 60 °C, leave 6–8 mm. Fix one end rigidly, slot the other.
  • 4. Cut on site if needed. Use carbide or diamond tools; never abrasive wheels that overheat the resin. Seal all cut edges within 30 minutes.
  • 5. Inspect. Walk the deck, check clip torque, confirm no panel flexes beyond L/150 under your design load.

Do's and Don'ts

DoDon't
Use SS316 clips in chloride / marine serviceWeld FRP panels — impossible and dangerous
Seal all cut edges with resin gel-coatMix stainless clip alloys on one deck
Allow thermal expansion gapsOvertorque bolts — strip the grid or crack the bar
Wear PPE when cutting (dust contains glass fiber)Stand on unsupported panel edges during install

For stamped installation drawings and clip schedules for your project, send us the span drawing — we return them within 48 hours, free for projects over 50 m².

Can you walk on GRP grating during installation?

Only on panels that are fully clipped at all supports. Unclipped or half-clipped panels can flex unexpectedly — treat the deck as out of service until final torque check is complete.

What bolts do I use to fix GRP grating?

Use SS304 G-clips indoors, SS316 in chloride / marine / food-grade washdown. M8 clips for 25-38 mm panels, M10 for 50 mm and above. Torque 8-22 N·m depending on size.