ISO 9001 Certified · FRP/GRP Grating Manufacturer · Since 2004 · Exporting to 45+ Countries

FRP Grating Material Properties

Fire, electrical, thermal, mechanical and section-property data for molded and pultruded FRP grating

Fire & Flame Performance

ASTM E-84 tunnel test and self-extinguishing ratings

Most molded FRP products achieve flame spread index ≤ 25 (Class A/B per E-84) and are self-extinguishing per ASTM D-635.

Resin SystemFlame Spread (E-84)Smoke / BehaviorCertification Notes
ZeAll VE (vinyl ester)≤ 25Self-extinguishing (D-635)DNV GL TAF000003C; ABS Type Approval; SGS & Intertek tested
ZeAll FDA (food-grade iso)≤ 25Self-extinguishing (D-635)USDA Approvable; antimicrobial
ZeAll ISO (improved iso)≤ 25Self-extinguishing (D-635)SGS & Intertek tested
ZeAll FR (extra FR vinyl ester)≤ 10Self-extinguishing (D-635)Lowest flame spread offered; SGS & Intertek tested
ELS (low-smoke)≤ 25Smoke developed ≤ 100; fuel contribution = 0DNV GL TAF000003C; SGS & Intertek tested
ZeAll Super VE (custom VE)Non-FR unless specifiedUp to 400°F (204°C) serviceSolvents / oxidizers / ClO₂ / NaOCl
ZeAllgrate Molded VE / ISO / FF≤ 25Smoke developed ≤ 450 (Class A)Flame impinged on top AND bottom; ABS Class ships

ZeAll FR vinyl ester offers the lowest flame spread (≤10). ELS is a low-smoke, zero-fuel-contribution grade. HLC molded grating: E-84 ≤ 25, Class 1 fire rating. Source: Industry reference Molded Catalog p.2,7; ZeAllgrate Molded Metric Brochure p.2.

Electrical Properties

Non-conductive grating with optional conductive (anti-static) surface

Fiberglass grating is electrically non-conductive by nature — a key safety benefit over steel in live electrical areas.

Baseline Insulation

FRP grating provides inherent electrical insulation. Arc resistance 120 s; dielectric strength 35 kV/in lengthwise; dielectric constant 5 @ 60 Hz (pultruded structural shapes).

Conductive Surface (NFPA 77)

For flammable/vapour atmospheres, specify a conductive surface: average surface resistivity 2.5×10³ – 1×10⁶ Ω per lineal foot; average resistance to ground < 10⁸ Ω.

Conductive Surface ParameterValue (per NFPA 77,2000 ed.)
Average surface resistivity2.5 × 10³ – 1 × 10⁶ Ω / lineal foot
Average resistance to ground< 10⁸ Ω
Grounding attachmentsRecommend ≥ 4 ground points, one at each corner

Source: Industry reference Molded Catalog p.2, p.8; Structural Shapes Brochure p.7.

Thermal Properties & Service Temperature

Low thermal conductivity and continuous-use temperature limits

FRP has low thermal conductivity — comfortable to the touch and an insulator against process heat.

Resin / SystemMax Continuous Service TemperatureEquivalent
ZeAll VE & pultruded VEFR180°F82°C
ZeAll ISO, ZeAll FDA, ZeAll FR & pultruded ISOFR150°F66°C
ZeAll Super VE (custom formulations)Up to 400°F204°C

ZeAll Super VE custom resins suit elevated-temperature service (solvents, oxidizers, ClO₂, NaOCl, liquid desiccants); they are non-fire-retardant unless specified. Source: Industry reference Molded Catalog p.2,7,19.

Statistical Design-Value Method

ASTM D7290 — characteristic (minimum) values

For engineering design, use characteristic minimum values, not "typical" averages.

Characteristic Value

Per ASTM D7290, the characteristic design value is typically the mean minus 2–3 standard deviations — a lower-bound value, not a mean.

Engineering Use

Industry reference recommends minimum or characteristic values for design. "Typical" values are not recommended for use by professional engineers; they describe material behaviour, not allowables.

Source: Industry reference ZeAllgrate Molded Metric Brochure, p.4.

Typical Coupon Mechanical Properties

Structural Shapes pultruded structural shapes (ISOFR / VEFR)

L.W. = lengthwise (along pultrusion / bearing bars); C.W. = crosswise. These are typical coupon values for pultruded structural profiles.

PropertyStandardLengthwise (L.W.)Crosswise (C.W.)
Tensile stressASTM D-63830,000 psi7,000 psi
Tensile modulusASTM D-6382.5 × 10⁶ psi0.8 × 10⁶ psi
Compressive stressASTM D-69530,000 psi15,000 psi
Compressive modulusASTM D-6952.5 × 10⁶ psi1.0 × 10⁶ psi
Flexural stressASTM D-79030,000 psi10,000 psi
Flexural modulusASTM D-7901.8 × 10⁶ psi0.8 × 10⁶ psi
Modulus of elasticity (full section)—2.8 × 10⁶ psi—
Shear modulus—0.450 × 10⁶ psi—
Short beam shearASTM D-23444,500 psi—
Punch shearASTM D-73210,000 psi—
Notched Izod impactASTM D-25625 ft-lb/in4 ft-lb/in

Physical & Electrical Coupon Properties

PropertyStandardValue
Barcol hardnessASTM D-49545
24-hour water absorptionASTM D-5700.45% max
DensityASTM D-7920.062–0.070 lb/in³ (≈1.72–1.94 g/cm³)
Coefficient of thermal expansion, lengthwiseASTM D-6968 × 10⁻⁶ in/in/°C (≈14.4 × 10⁻⁶ /°F)
PropertyStandardValue
Arc resistanceASTM D-495120 seconds
Dielectric strengthASTM D-14935 kV/in (lengthwise); 200 volts/mil (parallel to fiber)
Dielectric constantASTM D-1505 @ 60 Hz

Source: Industry reference Structural Shapes Brochure (Part No. 883102), p.7 "Typical Coupon Properties".

Molded Grating · Section Properties (Imperial)

Industry reference — per ft of width (in² / in⁴ / in³)

A = cross-sectional area, I = moment of inertia, S = section modulus.

Style (depth × mesh)A (in²)I (in⁴)S (in³)
5/8" × 1"×4" rect2.110.070.22
1" × 3/4"×4" (Ecograte62)3.580.2980.573
1" × 1"×4" rect2.570.220.43
1" × 1-1/2" sq1.710.140.29
1" × 2" sq1.270.110.21
1-1/4" × 1-1/2" sq2.160.320.48
1-1/2" × 1-1/2" sq2.850.510.65
2" × 2" sq2.880.960.94
HLC 1-1/2" × 1"×2"7.451.391.80
HLC 2" × 1"×2"10.263.43.27

Source: Industry reference Molded Grating Catalog, p.5–6, p.12–13.

Molded Grating · Section Properties (Metric)

ZeAllgrate Molded — per m of width (mm² / mm⁴ / mm³)

Standard panel matrix with open area and weight.

Thickness × MeshA per m (mm²)I per m (mm⁴)S per m (mm³)OpenWeight (kg/m²)
25.4 mm × 38.1 sq3.62 × 10³1.91 × 10⁵1.56 × 10⁴70%12.7
25.4 mm × 25.4×101.6 rect5.44 × 10³3.00 × 10⁵2.31 × 10⁴69%13.7
38.1 mm × 38.1 sq6.03 × 10³6.96 × 10⁵3.49 × 10⁴70%18.6
38.1 mm × Mini-Mesh7.98 × 10³9.75 × 10⁵4.26 × 10⁴44%22.0
50.8 mm × 50.8 sq6.09 × 10³13.11 × 10⁵5.05 × 10⁴72%19.5

25.4 mm × 25.4×101.6 rectangular mesh is grit-surface only. Mini-Mesh meets ADA (12.7 mm open mesh + slip resistance, regardless of travel direction). Source: Industry reference ZeAllgrate Molded Metric Brochure, p.3.

Design Values & Material Certificates

What these data are — and what to verify on your COA

Pultruded coupon values: the mechanical properties above (tensile, compressive, flexural, shear, impact) are typical coupon values for pultruded structural shapes in ISOFR/VEFR resins, transcribed from the Industry reference Structural Shapes brochure. They describe unidirectional pultruded performance.

Molded grating differs: molded grating contains roughly 33% glass (vs. ~70% for pultruded) and is bi-directional, so its specific laminate tensile / flexural / compressive numbers are lower and not interchangeable with the Structural Shapes coupon table. The molded catalogs publish section stiffness (A, I, S, EI) and load/span tables, not a dedicated coupon property sheet.

ZeAllgrate COA: for your exact resin, thickness and mesh, the controlling tensile (ASTM D638), flexural (ASTM D790), compressive (ASTM D695), specific gravity (ASTM D792) and water absorption (ASTM D570) values are supplied on the material certificate (COA) shipped with each batch. Share your resin system and we will provide the matching certificate and test report before order.

Data Sources

  • Industry reference Fiberglass Molded Grating & Products Catalog — fire ratings, electrical, thermal, molded section properties.
  • Industry reference ZeAllgrate Molded Metric Brochure — ASTM D7290 method, metric section matrix.
  • Industry reference Structural Shapes Brochure (Part No. 883102), p.7 Typical Coupon Properties. PDF
  • Industry reference ZeAll Pultruded Industrial Grating — Load Tables (resin systems VEFR / ISOFR). PDF

Request Your Material Certificate (COA)

Tell us your resin system, thickness and mesh — we return the matching certificate of analysis and load test report within 24 hours.